I’ve done a lot of research on how to finish oak so that I can complete my DIY bathroom vanity (which is made out of Red Oak).

In my last post, Understanding Wood Finishing: 10 Things I’ve Learned, I shared with you all of the exciting “new” products I discovered, like wood dyes and tips on how to use them.

I say “new” products because they’re not new at all.

Dyeing wood has been around for ages, but it’s new to me. As a DIY furniture painter, my experience with wood has been pretty limited. Who needed to know about wood when all you’re doing is painting it, right??

But it’s always bothered me that I didn’t know more. I couldn’t wait to get into my garage and start experimenting with some of the wood dyes because I knew the results would be dramatic!

Lately, I’ve had this intense desire to master the art of woodworking, building, construction, the understanding of wood, and recently, the desire to understand how to finish wood properly, too!

Let’s just call this “taking it to a whole ‘nutha level.”

Anyhow, after buying some exciting new products, I couldn’t wait to get started.

Today’s post is showing you how I learned to dye wood and use liming wax (along with some tips for alternative white grain fillers).

I was so excited by these results that I started texting everyone I know to show them pictures. HA!

What a DIY nerd….

Okay, on to the tutorial!

On the Go? Listen to This Blog Post: Push Play

I’ve added something new to the blog: audio! Maybe you don’t have time to read the entire post, but you can sure listen, can’t you? Go ahead and try. 😉
How to use wood dyes to create a richer color and use liming wax to highlight the grain - Thrift Diving

SKIP AROUND THIS POST

No time to read this entire tutorial? Click to skip around!

Introduction
STEP 1: Prepare a Sample Board
STEP 2: Wet the Wood With Distilled Waer to Raise the Grain
STEP 3: Sand the Wood With 150-grit Sandpaper
STEP 4: How to Mix Water-Based Wood Dyes
STEP 5: Apply the Wood Dye with a Rag, Brush, or Sponge
STEP 6: Add a Very Thin Coat of Shellac Sanding Sealer
STEP 7: Add a Thin Coat of Briwax Liming Wax
STEP 8: Use Clear Wax to Remove the Liming Wax
Things You Need to Know
What’s Next in Finishing this Red Oak Bathroom Vanity
PIN THIS Article
Subscribe

How to Dye Wood and Use Lime Wax to Finish Oak

Materials Needed:

STEP 1: Prepare a Sample Board

The other day when I stopped by the Woodworking supply store, I took some time to leaf through the books. One of them had an awesome suggestion. It suggested that before you work on your real project piece, you should create a sample board on which to practice all of your wood finishes.

I would highly recommend you do the same before attempting to use try this wood finishing technique on your real projects.

I’m building a DIY bathroom vanity and I’ve done a gazillion sample boards just to finally figure out what technique and shade looks best!

Anyhow, to prepare a sample board, get a long piece  Red Oak from The Home Depot. It doesn’t have to be super wide. Just wide enough so you can easily work on it and see the pattern.

The reason I’m using Red Oak is because it has an open pores that make it perfect for accenting grain!

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 500
The book recommended cutting small kerfs (a kerf is a slit made from cutting) into your sample board to keep the samples separate from one another. This prevents the dyes from soaking into each other. It’s totally optional but very helpful.

You can also use painters tape. But be sure to use some space between the samples so they don’t bleed.

You can see here how the kerfs keep my samples separated.

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 503

 

STEP 2: Wet the Wood With Distilled Water to Raise the Grain First

When water touches wood, especially wood that has a lot of open pores, like Red Oak, it will raise the grain.

To give you an idea of what Red Oak looks like BEFORE and AFTER you raise the grain, this is a great picture to show you.

Notice on the bottom of this board, the grain is more closed and flat? It’s still porous, but smoother.

But the top, after I wiped on water, then wiped it off and let it dry, suddenly the grain is more pronounced and rough.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak-379

 

When you use water-based wood dyes, which are dissolved in water, this is what would happen to your wood when you apply them.

The grain would become open and more pronounced. And I believe this can affect the quality of the finish you get.

So to thwart the grain raising, you should pre-wet your wood first when using water-soluble wood dyes.

Just take a small brush or rag, wipe the water on.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 536

 

Use a clean towel to wipe the water off, and then let it dry about 30 minutes or so, or longer if the wood still looks wet.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 539

 

Be sure to use distilled water (water that is boiled to remove the contaminants) when using wood dyes so that no contaminants can interfere with how your dyes turn out.

You can just pick up a jug from your regular grocery store for a little over a buck.

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 562

 

STEP 3: Sand the Wood With 150-grit Sandpaper

Now that the wood is dry and the grain is raised, you just sand down the grain again.

It’s interesting to know that the grain on wood only really raises once. Isn’t that amazing??

So after you raise the grain and then sand it back down, if you put water or water-based products on it again, it won’t raise much. Good to know!

Anyhow, to sand it smooth, I discovered this little tip:

Take a pencil and draw a figure or markings on your wood.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 508

 

Start sanding with your 150-grit sandpaper.

You’ll see the pencil marks start to disappear.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 511

 

Once you’ve sanded down enough to where you can’t see the pencil markings anymore, you know it’s time to switch to the next finer grit sandpaper.

At that point, you’ll want to place another set of pencil markings and use the 180-grit sandpaper (which is finer) until you can’t see the markings anymore.


How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 513

 

Be sure to wipe up (or vacuum) all the dust, because you don’t want that getting stuck in your finish!



How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 520

 

STEP 4: How to Mix Water-Based Wood Dyes

Now that your wood is smooth again, it’s time to mix your dyes.

Every woodworking site I researched all suggested using water-based wood dyes (also known as aniline dyes, although apparently, they don’t contain the chemical aniline anymore). The reason why they’re easier to apply is because they don’t obscure the grain of the wood as much as other dyes, and are safer (since you’re only mixing them with water and not other solvents).

At the woodworking shop the other day I picked up a few of these TransFast powdered dyes (about $12.50 each).

 

Understanding Wood Finishing - Thrift Diving - 252

 

I decided to test out the Grey and Ebony on my sample board to see which one I may want to use for my DIY bathroom vanity.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 564

 

How to Mix Powdered Wood Dye

What the manufacturer recommends for these Homestead TransFast dyes is to mix 1 ounce of powdered dye in 2 quarts of hot (not boiling) water. (Hot water helps the powdered dye to dissolve better, but let the mixture cool down before you use it).

However, everything I’ve read online suggests mixing 1 oz. of dye in 1 quart of water. (The small containers of wood dye that I bought are exactly 1 ounce, by the way).

You can mix even smaller amounts for sample boards.

 

How to Dye Wood - Mix water-based aniline dyes with hot water but not boiling water

 

However, I later learned that you should always mix it stronger than the manufacturer suggests.

For example, instead of mixing 1 oz. of powdered wood dye in 1 quarts of hot water, try mixing 1 oz. of dye in 1 pint of hot water.

It’s not an exact science because it’s going to depend on how dark or light you want your wood to be (don’t over mix, however, or you’ll end up with a bunch of dye at the bottom and it could make your wood powdery).

But the reason you’d want to mix it more concentrated is that you can always later add water to lighten it to the exact shade you want.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 571

 

I didn’t do this step, but it’s recommended to filter your mixed dye at his point, using a paint filter or maybe a coffee filter.

Good to know: Wood dye will last about 6 months once it’s mixed. Store it in a cool, dark place in a covered container or jar. In the powdered form, it lasts indefinitely. Check out these FAQ about the Homestead aniline dyes website.

 

STEP 5: Apply the Wood Dye with a Rag, Brush, or Sponge

The first batch of wood dye that I mixed was waaaayyy too light.

I ended up adding more powdered dye, but honestly, I still don’t think it was as concentrated as it could have been because it went on lighter than I expected.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 568

 

Since the color was too light, adding more powdered dye solved that problem.

If the color is too deep or intense on your wood, you can always wipe it with a wet cloth and instantly lighten it up (you can’t change the color of pigments stains very much once you’ve applied them). This is the good thing about water-based dyes: they dry more slowly, so you have more room to change their color or intensity.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 569

 

Anyhow, after making it a bit more concentrated, I noticed that it did start to get darker.

Once it’s all covered, wipe off the excess.


How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 572

 

Next, I used the Ebony wood dye to do another side of the sample board. I mixed this one more concentrated, so you can see how much more rich the color became immediately.

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 573

 

How to Test How Dark Your Wood Will Be Once It Dries

Once the water in the wood dye mixture evaporates, it will leave behind the wood dye and your wood will look a bit darker.

But until the water evaporates, you have no way of really knowing how dark your project will be.

One way to test this is by wiping on a little bit of mineral spirits.

Water-based wood dyes don’t react to mineral spirits, so it won’t disturb your wood dye one bit.

What it will do is slightly darken the surface so you can “test” to see how dark the color will be once it dries.  At that point, you can either decide to darken the dye by layering on a more concentrated color or you can lighten the dye by wiping it off with a wet towel. That’s a lot of flexibility right there!

Pretty cool, huh??

I didn’t test mine because I didn’t learn that little trick until after-the-fact, but you can bet I’ll try it the next time I do a test board with these wood dyes!

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 574

 

What’s the Difference Between Wood Dyes and Pigment Stains?

Another thing I want to point out is the difference between wood dyes and wood pigments (such as Minwax stains we all know).

Wood stains, such as Minwax, have pigments in them that simply lie on the wood, in cracks and crevices in the wood.

Wood dyes penetrate and actually color the wood.

Since this was my first time experimenting with wood dyes, the difference was so clear when I saw that the wood dyes didn’t obscure the grain of the wood.

Below, you can see that the grain is still visible and open, not filled with pigmented color.

This is actually pretty important because since I’m using a liming wax to highlight that pretty grain, I want the grain to be open and ready to accept the wax, not filled with pigments that are already taking up space in the grain.

I couldn’t wait to get some lime wax into those grains!

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 577

 

STEP 6: Add a Very Thin Coat of Shellac Sanding Sealer

 

It’s best to let your wood dry for about 24 hours. It might seem to be dry, but it can still be wet down inside the wood, so you shouldn’t rush this process.

Now it’s time to add a very thin layer of dewaxed shellac sanding sealer to help seal in the dye.

 

Dewaxed SealCoat sanding sealer helps seal in water-based wood dyes before adding a topcoat or waxing.

 

One reason why this is important is because–remember–these dyes are water-soluble.

If you add a coat of water-based polyurethane over water-soluble dye, it will start to active the dye again and it can mess up your dye. (In this case, we’re going to be using lime wax, but just so you know….).

But when you add a coat of sealer, you’re essentially locking in that dye, creating a barrier for what comes next.

Plus, sanding sealer doesn’t obscure the grain, so it will still allow us to use lime wax to create a nice, highlighted grain.

No need for a brush–only use a clean, lint-free cloth and put a very light coat with the grain.

Let the sealer dry for about 2-4 hours.

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 583

 

STEP 7: Add a Thin Coat of Briwax Liming Wax

Liming wax is amazing stuff.

People use liming wax to add white to the grains of very porous wood, like Red Oak, creating this gorgeous highlight in the grain.

If you were to ask me what consistency liming wax has, I would say it reminds me of Noxema.

Remember that skincare product that every teenager used religiously? HA!!

Well, it looks and feels exactly like that!

 

Understanding Wood Finishing - Thrift Diving - 268
You don’t need a lot, so don’t slap on tons of it.

Just use a soft, lint-free cloth and push it into the grain.

You’ll start to see this awesome effect taking place right before your eyes: it’s the grain coming alive! 🙂

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 586

 

Leave the wax on for 3-5 minutes.

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 589

 

STEP 8: Use Clear Wax to Remove the Liming Wax

When I tried to wipe these boards clean, the liming wax left a whitewashed look, which is fine if that’s the look you’re going for.

However, because I don’t want to leave the boards white and I only want the grain to be white, I need to remove the liming wax from the rest of the board.

Because I used that thin coat of dewaxed shellac sanding sealer to create a barrier between the wood dye and the liming wax, it’s easier to remove the liming wax.

And to help me do it, I used use clear wax.

I didn’t get a great picture of this step, but what you do is rub clear wax over the lime wax, and it will start to come off very easily.

The liming wax stays put in the grain, leaving this gorgeous highlighted grain in the Red Oak!

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 590

 

What I’m left with is beautifully stained wood with liming wax highlighting the grain, creating the most beautiful Red Oak I have ever seen!

Since these are sample boards, I ended it at this point, but if this were a real project (such as my DIY bathroom vanity), I would come back after 24 hours and add another coat of clear wax and buff it to a shine.

Wax should be reapplied every 6 months to keep the wood protected and in good shape.

NOTE: If you’re using your wood in a moist place, like a bathroom, keep reading below (see Things You Should Know) to find out why wax wouldn’t be a good option to create this look.

 

How to Dye Wood and Use Liming Wax to Accent the Grain

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 592

 

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 595

How-to-Stain-and-Dye-Wood-Lime-Wax-Oak - 594

Things You Need to Know

There are a few things to know about using wood dyes. Don’t forget that:

  • Dyes are more likely to fade. Using dyes wouldn’t be a good idea on pieces of furniture or wood projects that will be used in direct sunlight or outdoors. Since my vanity isn’t in direct light, it’s fine, but keep this in mind for your furniture piece.
  • You will not be able to add any other topcoat. When you use wax, you cannot use any other type of topcoat. You can only use wax on top. Therefore, if you are hoping to create the look of a white highlighted grain and you want to use a water-based topcoat, you would either have to use a water-based white grain filler or use white paint so that you could use a more durable topcoat. (This is likely the route I’ll have to go for my DIY bathroom vanity). Varathane just came out with a new product called Wood Grain Enhancer, but I think it’s so new that I can’t find it anywhere in stores, not even on Amazon! GASP! Looks like it cleans up easily with water, so this may be a good option for creating that pretty contrast in the oak and then being able to use a great water-based topcoat. I’ll keep you posted on this new product as soon as I’m able to try it out!

Varathane Wood Grain Enhancer to accent wood grain

 

  • Use a UV protective sealer if you’re not waxing. If you’re not highlighting the grain of the wood with liming wax (and you’re using a white grain filler or white paint) then be sure to use a UV protective top coat that can help protect the wood from fading.
  • Dyes look best on unfinished wood. Not that I’ve used them enough to know first hand, but from my research, I’ve learned that wood dyes work best on unfinished bare wood because they’ve not been contaminated with anything else. This could be good for small projects you might make, picture frames, DIY wooden journals, or any other wood craft or DIY project you make.

 

What’s Next in Finishing This Red Oak Bathroom Vanity

I can’t tell you how nervous I am about finishing this vanity!

As I mentioned above, since this is a bathroom vanity, where there are moisture and water, I’ll want to use a more durable finish. Wax probably wouldn’t work in this case if I want this vanity to last long.

 

 

How to build a DIY bathroom vanity - Making Cabinet Doors - Thrift Diving

 

Have you ever finished oak before and using wood dyes and liming wax to create beautiful wood?

Leave a comment below and let’s chat about it!

How to use wood dyes to create a richer color and use liming wax to highlight the grain - Thrift Diving

Did you enjoy this post? Click to SAVE IT on Pinterest!

How to Use Wood Dye and Accent the Wood Grain

SIGNATURE

Download the 5 freebies!

Thrift Diving inspires women to decorate, improve, and maintain their home themselves...using paint, power tools, and thrift stores! Use these 5 printables, checklists, and ebooks to get started!

Now go check your email for those freebies! Powered by ConvertKit

Love this post? Share it! :)

Similar Posts

26 Comments

  1. Hi, would you please share which dye color was used on each of the samples at the end of your article? I’m so intrigued!

  2. Leesa Wachsman says:

    Hello, OK…I have a stairway and upstair landing with hand scraped red oak that we finished with Briwax Tudor Brown over 20 years ago and they have been wonderful. BUT…I am wanting to change my look and get rid of the golden colors. I have attempted to put Briwax Ebony over a top stair tread to see what it would do. And….it does the job…but I was considering using the Liming Wax to tone it down. Do you think I could you the Liming wax over the Ebony? Should I just try it??

  3. hi there –

    so, i’m most intrigued by how the natural red oak reacted to the water / liming wax. do you have another article / post that shows images of the undied red oak with liming wax?

    thanks,

    john

  4. I learned the hard way that when you mentioned a “thin” coat of sealant to protect the dye, it really is a “thin” coat. I made the mistake of following the sealant directions and applied three coats (super durable table!). Now I don’t have any pores that are really open enough on this red oak table to hold the lining wax. It all really just wipes off. So disappointed as this was to be the crowning moment for this table project!

  5. I tried the white wood enhancer and it was terrible. I &ollowed the instructions – opening the grain with a wire brush – but it it’s very gritty and sits ON the grain rather than seeping into it. Wiping it removed 95% of it, leaving a barely noticeable effect. . I wasted hours on the wood enhancer, finally gave up and used a watered down whitepaint – worked like a charm!

    1. Hey there, Clair! Since writing this post, I have tried the Wood Grain Enhancer and I completely agree with you! I need to amend this post and state that very fact: that it sucks! It wasn’t a good product at all. They’d sent me a couple cans to test out and the same thing happened to me. It just sat on the surface and didn’t really do anything for the wood! I saw this company at a blogging conference over the summer last year and I actually told their reps that I didn’t like it when I saw them doing demos with it. I walked up and was like, “Yeaaaaah, I kinda don’t like this product.” Sorry you had a crappy experience, too! I have when products don’t live up to their hype!

      1. Hi Serena!
        I’m glad you gave them appropriate and fair feedback, it’s a shame they didn’t take it to heart. I don’t know how it made through their approval process, and it’s not cheap ($30 Canadian)! I wasn’t sure how old your post was but had hoped to prevent you from wasting time on it too! I bought Liberon Liming Wax a few months ago and really like it – you’re right, it’s texture is exactly like the Noxema I used in high school! The good ole days… Anyway, I enjoyed your post and was impressed to see we have the same dedication to research! My focus the last two years has been on the woodworking/building side – I found I enjoy building and fixing broken furniture more than just painting, but it’s a lot more time consuming! I’ll check out your blog for more helpful info!

        Clair

        1. My blog is a bit out of date, but will be posting my latest secretary desk (fix, broken pieces, add new leather insert, strip, sand, stain, liming wax) soon!

Leave a Reply

Your email address will not be published. Required fields are marked *